Mineral: |
Calcite |
Reference: |
LJ20 |
SCM Type: |
DDL - Diffuse Double Layer
|
Ionic Strength: |
0.0 mol/L of
|
Site Type: |
»Ca-OH |
PZC: |
|
pK1: |
12.2 |
pK1°I=0 (Conversion to I = 0): |
12.20 |
pK12.31 nm−2 (normalized): |
12.53 |
pK2: |
|
pK2°I=0 (Conversion to I = 0): |
|
|
Site Density in nm-2: |
4.9501 |
Original Site Density: |
8.22 µmol / m² surface
|
Solid/Liquid Ratio in g/L: |
|
pH Range: |
|
Temperature in K: |
298.15 |
Method for Site Density: |
Literature |
Method for Protolysis: | Literature |
Fit Method: |
Comment: |
SSD taken from [SPJL11]; pK values from [VCSW93] (pK1 from reaction >CaOH<2+> = >CaOH° + H<1+>; pK2 from reaction >CO3H° = >CO<3-> + H<1+> in [VCSW93]) |
|
Mineral: |
Calcite |
Reference: |
LJ20 |
SCM Type: |
DDL - Diffuse Double Layer
|
Ionic Strength: |
0.0 mol/L of
|
Site Type: |
»CO3H |
PZC: |
|
pK1: |
|
pK1°I=0 (Conversion to I = 0): |
|
|
pK2: |
4.9 |
pK2°I=0 (Conversion to I = 0): |
4.90 |
pK22.31 nm−2 (normalized): |
4.57 |
Site Density in nm-2: |
4.9501 |
Original Site Density: |
8.22 µmol / m² surface
|
Solid/Liquid Ratio in g/L: |
|
pH Range: |
|
Temperature in K: |
298.15 |
Method for Site Density: |
Literature |
Method for Protolysis: | Literature |
Fit Method: |
Comment: |
SSD taken from [SPJL11]; pK values from [VCSW93] (pK1 from reaction >CaOH<2+> = >CaOH° + H<1+>; pK2 from reaction >CO3H° = >CO<3-> + H<1+> in [VCSW93]) |
|